Product classification
GH4033 (GH33) high-temperature alloy
GH4033 high-temperature alloy is based on nickel-chromium, with the addition of aluminum and titanium to form γ phase dispersion-strengthened alloy. It has sufficient high-temperature strength at 700-750°C and good oxidation resistance below 900°C. This alloy has good heating workability and is mainly supplied as hot-rolled bars and discs, used in engine rotor parts.
Classification:
Key words:
Superalloy | Inkenel | Hastelloy | Inkloy | Precision Alloy Series
Product Parameters
GH4033
Chinese grade: GH4033 (GH33) high-temperature alloy
Foreign grade: ЭЙ437Б, ХН77ТЮР (Russia)
1.Overview of GH4033 high-temperature alloy:
GH4033 high-temperature alloy is based on nickel-chromium, with aluminum and titanium added to form a γ-phase dispersion-strengthened alloy, which has sufficient high-temperature strength at 700~750℃ and good oxidation resistance below 900℃. This alloy has good heating performance and is mainly supplied as hot-rolled bars and disc blanks, used in engine rotor parts.
1. Chemical composition of GH4033 (GH33): see Table 1-1:
Table 1-1
| C≤ | Si≤ | Mn≤ | P≤ | S≤ | Cr≥ | Ni≥ | Mo≥ | Cu≤ |
| 0.03-0.08 | 0.65 | 0.35 | 0.015 | 0.007 | 19.0-22.0 | Remainder | - | - |
| Others | N≤ | Al≤ | Ti≤ | Fe≤ | B≤ | Ce≤ | W≤ | Nb≤ |
| - | 0.60-1.00 | 2.40-0.80 | 4.00 | 0.01 | 0.01 | - | - |
2. Heat treatment system of GH4033 (GH33):
For rotating parts, the hot-rolled bar is heated to 1080℃±10℃, air-cooled + 700℃±10℃, 16h, air-cooled. For ordinary load-bearing parts, the bar and cold-drawn bar are heated to 1080℃, 8h, air-cooled + 700℃ or 750℃, 16h, air-cooled. For ring blanks and forged discs, the temperature is 1080℃, 8h, air-cooled + 750℃, 16h, air-cooled.
3. Melting and casting process of GH4033 (GH33):
Melting is done using electric arc furnace, electric arc furnace + electroslag or vacuum arc remelting, non-vacuum induction furnace + electroslag or vacuum arc remelting, vacuum induction furnace + electroslag or vacuum arc remelting.
4. Other overview and special requirements of GH4033 (GH33):
This alloy is widely used in high-temperature components of turbine engines, mainly as turbine working blades, turbine discs, and other high-temperature load-bearing components. It is one of the alloys with mature usage experience both domestically and internationally. Attention should be paid to the recrystallization issue during hot rolling and forging, as it tends to form uneven and coarse grains, leading to coarse grain waste. Additionally, strict control of the production process is required to avoid the phenomenon of reduced plasticity at 700℃.
2.Physical properties of GH4033 (GH33):
1. Thermal performance of GH4033 (GH33):
(1) Thermal conductivity of GH4033 (GH33): see Table 2-1
Table 2-1
| θ/℃ | 100 | 200 | 300 | 400 | 500 | 600 | 700 | 800 | 900 |
| λ/(W/(m·C)) | 11.30 | 12.97 | 14.64 | 16.32 | 17.99 | 20.08 | 22.59 | 25.11 | 27.62 |
(2) Linear expansion coefficient of GH4033 (GH33): Table 2-2
Table 2-2
| θ/℃ | 20~100 | 20~200 | 20~300 | 20~400 | 20~500 | 20~600 | 20~700 | 20~800 | 20~900 |
| α/10-6C-1 | 11.56 | 12.30 | 13.17 | 13.79 | 14.52 | 15.07 | 15.62 | 16.30 | 17.15 |
2. Density of GH4033 (GH33): ρ=8.2g/c
3. Electrical performance of GH4033 (GH33): resistivity ρ=1.24×10-6Ω·m
4. Magnetic properties of GH4033 (GH33): The alloy is non-magnetic.
3.Chemical properties of GH4033 (GH33):
1. Oxidation resistance of GH4033 (GH33): Oxidation rate after 100h test in air medium: see Table 3-1
Table 3-1
| θ/℃ | Oxidation rate / (g/(m3·h)) |
Oxidation rate / (g/(m3·h)) |
Oxidation rate / (g/(m3·h)) |
Oxidation rate / (g/(m3·h)) |
| 25h | 50h | 75h | 100h | |
| 800 | 0.086 | 0.064 | 0.051 | 0.045 |
| 900 | 0.212 | 0.171 | 0.133 | 0.118 |
| 1000 | 0.732 | 0.491 | 0.376 | 0299 |
2. Metallographic structure of GH4033 (GH33): This alloy has a single-phase austenitic structure in the solid solution state, with trace amounts of TiC, TiN [Ti(C, N)].
4.Process performance and requirements of GH4033 (GH33):
1. This alloy has good hot working performance, with forging heating temperature at 1140℃ and final forging at 950℃.
2. The average grain size of this alloy is closely related to the degree of deformation of the forged piece and the final forging temperature.
3. Alloys can be argon arc welded in a solid solution state, and post-welding treatment should be carried out promptly to eliminate welding stress.
4. Surface treatment process: Parts that have been machined need to undergo electrolytic polishing. If mechanical polishing is used, the final polishing scratches should be consistent with the length direction of the blades.
5. The heating rate for solid solution treatment of parts should not be too fast; a step heating curve can be used.
五、GH4033(GH33) varieties, specifications, and supply status:
1. Variety classification:GH4033(GH33) seamless pipes, steel plates, round steel, forgings, flanges, rings, welded pipes, steel strips, wire materials, and matching welding materials.
2. Delivery status: Seamless pipes: solid solution + acid white, length can be customized; plates: solid solution, acid pickling, edge cutting; welded pipes: solid solution acid white + RT% flaw detection, forgings: annealed + turned; bars in forged state, surface polished or turned; strips delivered in cold-rolled, solid solution soft state, and descaled; wire materials delivered in solid solution acid pickled coil or straight bar form, solid solution straight bar fine polished state.