Product classification
GH3625/GH625 nickel-based high-temperature alloy
GH3625 is a solid solution strengthened nickel-based superalloy with molybdenum and niobium as the main strengthening elements. It has excellent corrosion resistance and oxidation resistance, good tensile and fatigue properties from low temperatures up to 980°C, and resistance to stress corrosion in salt spray environments. Therefore, it can be widely used in the manufacture of aircraft engine components, aerospace structural parts, and chemical equipment. The alloy has good processing and welding properties and can supply various forms such as plates, bars, pipes, wires, strips, and forgings.
Classification:
Key words:
Superalloy | Inkenel | Hastelloy | Inkloy | Precision Alloy Series
Product Parameters
GH3625
Chinese grade: GH3625/GH625 nickel-based high-temperature alloy
American grade: Inconel625/UNS NO6625
French grade: NC22DNb
German grade: W.Nr.2.4856
1.Overview of GH3625 nickel-based high-temperature alloy:
GH3625 is a nickel-based deformation high-temperature alloy with solid solution strengthening, primarily reinforced by molybdenum and niobium. It has excellent corrosion resistance and oxidation resistance, good tensile and fatigue properties from low temperature to 980℃, and is resistant to stress corrosion in salt mist atmospheres. Therefore, it can be widely used in the manufacture of aircraft engine components, aerospace structural parts, and chemical equipment. The alloy has good processing and welding properties and can supply various plates, bars, pipes, wires, strips, and forgings.
1. GH3625 material grade: GH3625 (GH625).
2. Similar grades to GH3625: Inconel625, UNS NO6625 (USA), NC22DNb (France), W.Nr.2.4856 (Germany).
3. Technical standards for GH3625 material:
4. Chemical composition of GH3625: see Table 1-1.
Table 1-1%
| C≤ | Si≤ | Mn≤ | P≤ | S≤ | Cr≥ | Ni≥ | Mo≥ | Cu≤ |
| 0.10 | 0.50 | 0.50 | 0.015 | 0.015 | 20.0-2300 | Remainder | 8.0-10.0 | 0.07 |
| Others | N≤ | Al≤ | Ti≤ | Fe≤ | Co≤ | V≤ | W≤ | Nb≤ |
| - | 0.40 | 0.40 | 5.00 | 1.00 | - | - | - |
5. Heat treatment system for GH3625: Bars: 950~1030℃, air cooling or water cooling; or 1090~1200℃, air cooling or water cooling solution treatment. Plates: 950~1030℃, air cooling; or 1090~1200℃, air cooling. Pipes: Recommended annealing temperature: 960~1030℃, air cooling or water cooling.
6. Specifications and supply status of GH3625: Bars with diameters of 25 to 80mm and plates with thicknesses of 0.8 to 10.5mm can be supplied, as well as seamless (welded) pipes with diameters of 6 to 40mm. Bars are delivered in a turned or polished state without heat treatment; plates are supplied after solution treatment and finishing; pipes are supplied after solution treatment and acid cleaning (or bright annealing).
7. Melting and casting process of GH3625: The alloy is produced using vacuum induction melting followed by electroslag remelting or vacuum induction melting followed by vacuum arc remelting.
8. Application overview and special requirements of GH3625: This alloy is used to manufacture components such as engine casings, guide blades, mounting edges, and fuel manifolds, and has passed practical application assessments, with a maximum service temperature of 950℃. The alloy exhibits some aging hardening phenomenon after long-term use at 550~700℃, leading to a slight decrease in alloy plasticity.
2.Physical and chemical properties of GH3625:
1. Thermal properties of GH3625:
(1) Melting temperature range of GH3625: 1290~1350℃[1].
(2) Thermal conductivity of GH3625: see Figure 2-1.
(3) Specific heat capacity of GH3625: see Figure 2-2.
(4) Linear expansion coefficient of GH3625: see Figure 2-3.
2. Density of GH3625: ρ=8.44g/cm3.
3. Electrical properties of GH3625: Alloy resistivity see Figure 2-4.
4. Magnetic properties of GH3625: The alloy is non-magnetic.
5. Chemical properties of GH3625:
(1) Oxidation resistance of GH3625: The alloy has excellent high-temperature oxidation resistance, and the weight change of the alloy after cyclic oxidation in air at high temperatures is shown in Table 2-1.
Table 2-1[1]
| Cyclic oxidation time/h | 100 | 200 | 300 | 400 | 500 | 600 | 700 | |
| Weight change/% | 980℃ | +0.086 | +0.065 | +0.065 | +0.048 | +0.021 | - | +0.030 |
| 1095℃ | -0.182 | -1.086 | -3.335 | -5.399 | -6.566 | -10.066 | - | |
Note: Cyclic oxidation heating for 15 minutes, cooling for 5 minutes constitutes one cycle.
(2) The corrosion resistance of GH3625 alloy has good resistance to seawater corrosion, as shown in Table 2-2. The alloy is also resistant to corrosion from various salt solutions. In addition, it has good resistance to nitric acid and phosphoric acid corrosion, and it also has considerable resistance to hydrochloric acid below boiling point and low concentration sulfuric acid.[2].
Table 2-2[1]
| Test Days | Sample Type | Weight Loss/g | Local Corrosion Degree | Test Days | Sample Type | Weight Loss/g | Local Corrosion Degree |
| In Static Seawater | In Flowing Seawater (0.61m/s) | ||||||
| 180 | Smooth With Gaps |
0.05 0.05 |
None None |
180 | Smooth With Gaps |
0.04 0.05 |
None None |
| 365 | Smooth With Gaps |
0.02 0.04 |
None None |
365 | Smooth With Gaps |
0.01 0.02 |
None None |
Note: The smooth sample refers to a flat sample with a circular weld of 6.4mm×100mm×300mm, annealed at 980℃ before welding. The sample with gaps is fixed at the center of the plate surface with a 32mm fiber gasket using bolts.
Three,Mechanical Properties of GH3625:
The performance specified by the technical standards for GH3625: See Table 3-1.
Table 3-1
| Variety | Tensile Properties | Durability | Hardness | ||||||
| θ/℃ | σb/MPa | σP0.2/MPa | δ5/% | θ/℃ | σ/MPa | t/h | δ5/% | ||
| Not less than | Not less than | ||||||||
| Bar① | 20 | 830 | 410 | 30 | 815 | 114 | 23 | 15 | HB≤290 |
| Plate② | 20 | 830 | 410 | 30 | 815 | 114 | 23 | 15 | HV≤305 |
| Bar | 20 | 830 | 410 | 30 | Q/3B 4078-1992 | - | |||
| Plate | 20 | 825 | 415 | 30 | Q/3B 4077-1992 | - | |||
| Pipe | 20 | 825 | 415 | 35 | Q/3B 4080-1992 | HRC≤25 | |||
① Standard Z9-0105-1990. ② Standard Z9-0104-1990 and GJB 3317-1998.
Four,Microstructure of GH3625:
1. Phase Transformation Temperature of GH3625:
2. Time-Temperature-Structure Transformation Curve of GH3625:
3. Microstructure of GH3625 Alloy: The microstructure of the alloy in the solid solution state is an austenite matrix with a small amount of TiN, NbC, and M.6C phase, after long-term aging at 650~900℃, the precipitated phases are γ", δ, M.23C6and M.6C. After long-term aging at 650~700℃, mainly γ" precipitates, which significantly improve the room temperature and high-temperature strength of the alloy, while plasticity decreases somewhat but remains at a high level; after aging at 780~850℃, mainly δ phase precipitates, although strength increases, the plasticity of the alloy decreases significantly. After aging at 900℃, only a small amount of precipitated phase remains, so the mechanical properties are similar to those in the solid solution state. The δ phase has an orthogonal structure of flaky Ni.3Nb, and exists in a needle-like Widmanstätten structure.[1,7].
Five,Process Performance and Requirements of GH3625:
1. Formability of GH3625: The alloy has good hot and cold forming performance. The forging heating temperature for steel ingots is 1120℃, the opening forging temperature is not lower than 1030℃, and the stopping forging temperature is not lower than 930℃; during die forging, the final deformation amount should not be less than 15%~20%. The rolling heating temperature is 1120~1160℃, the opening rolling temperature is not lower than 1050℃, and the stopping rolling temperature is not lower than 930℃, with a deformation amount of 25%~30% for cold-rolled semi-finished thin plates and not less than 30% for finished products. The quenching temperature for intermediate and finished products is 1100℃±10℃.[1,8].
2. Welding Performance of GH3625: The alloy has good welding performance and can be welded using tungsten electrodes or the alloy itself as filler in an inert atmosphere for argon arc welding, and can also be connected using brazing and resistance seam welding.
3. Heat Treatment Process for GH3625 Parts: Stress relief: 900℃; Annealing: 930~1040℃, 1h; Solution treatment: 1090~1200℃, air cooling or water cooling. When the alloy works at temperatures not exceeding 650℃, materials in hot-rolled, cold-rolled, or annealed states can be used as required. When the working temperature is above 650℃, components requiring good fatigue performance and tensile strength can use the annealing process, while those requiring good creep and durability can use the solution treatment.
4. Surface Treatment Process for GH3625: Remove the oxide scale from the alloy surface by first alkaline washing, then acid washing in a nitric acid-hydrofluoric acid-water solution.
5. Cutting and Grinding Performance of GH3625: Hard alloy or high-speed steel tools should be used. The cutting tools used should have a positive rake angle. Water-based coolants are recommended for high-speed cutting, while thicker coolants are recommended for low-speed cutting.
Six,Specifications and Supply Status of GH3625:
1. Variety classification: GH3625 seamless pipe, GH3625 steel plate, GH3625 round steel, GH3625 forgings, GH3625 flanges, GH3625 rings, GH3625 welded pipes, GH3625 steel strips, GH3625 wire and GH3625 matching welding materials.
2. Delivery status: Seamless pipe: solution + acid pickling, length can be specified; plate: solution, acid washing, edge cutting; welded pipe: solution acid pickling + RT% flaw detection, forgings: annealed + turned; bars in forged and rolled state, surface polished or turned; strips delivered in cold-rolled, solution soft state, deoxidized; wire delivered in solution acid washed coil or straight bar form, solution straight bar fine polished state.
Previous Page
Previous Page
GH3536/GH536 nickel-based high-temperature alloy
Related Products
Product Consulting
Leave your contact information to get a free product quote!