GH600 is an early-developed nickel-chromium-iron-based solid solution strengthened alloy, which has good high-temperature corrosion resistance and oxidation resistance, excellent cold and hot processing and welding process performance, and satisfactory thermal strength and high plasticity below 700°C. The alloy can be strengthened through cold processing and can be joined using resistance welding, fusion welding, or brazing. It is available in cold-rolled thin sheets, hot-rolled thick plates, strips, wires, bars, discs, ring blanks, and ring forgings, making it suitable for manufacturing oxidation-resistant parts that bear low loads below 1100°C.
Classification:
Key words:
Superalloy | Inkenel | Hastelloy | Inkloy | Precision Alloy Series
Product Parameters
GH600
Chinese grade: GH600/GH3600 nickel-based high-temperature alloy
American grade: Inconel/Inconel600
1.Overview of GH600 nickel-based high-temperature alloy:
GH600 is an early developed nickel-chromium-iron-based solid solution strengthened alloy, which has good high-temperature corrosion resistance and oxidation resistance, excellent cold and hot processing and welding process performance, and satisfactory thermal strength and high plasticity below 700°C. The alloy can be strengthened by cold working and can be connected by resistance welding, fusion welding, or brazing. It can be supplied in the form of cold-rolled thin plates, hot-rolled thick plates, strips, wires, bars, discs, ring blanks, and ring forgings, suitable for making oxidation-resistant parts that bear low loads below 1100°C.
1. GH600 material grade: GH600.
2. Similar grades to GH600: Inconel, Inconel600 (USA).
3. Technical standards for GH600 material:
4. Chemical composition of GH600: see Table 1-1.
Table 1-1
| C≤ | Si≤ | Mn≤ | P≤ | S≤ | Cr≥ | Ni+Co≥ | Mo≥ | Cu≤ |
| 0.15 | 0.50 | 1.00 | 0.040 | 0.015 | 14.0-17.0 | 72.0 | - | 0.50 |
| Others | N≤ | Al≤ | Ti≤ | Fe≤ | Co≤ | V≤ | W≤ | Nb+Ta≤ |
| - | 0.35 | 0.50 | 6.0-10.0 | - | - | - | 1.00 |
Note: 1) The aerospace material standard BZ-44-9003B-0 stipulates ω(C)≤0.10%, ω(P)≤0.020%, ω(Nb)≤1.00%.
2) The Fuhai High-tech 1995-13 standard stipulates ω(P)≤0.025%, ω(Nb)≤1.00%.
5. GH600 heat treatment system: Plates: 1010~1050℃, 3~5min/mm, air cooling; Strips: 1010℃±10℃, air cooling; Wires: 1065℃±10℃, air cooling. Bars and ring parts are inspected and tested at 1010℃±10℃, air-cooled solution treatment.
6. Specifications and supply status of GH600: Various specifications of plates, bars, forgings, strips, wires, discs, ring blanks, and ring forgings can be supplied. Bars are supplied in forged and rolled state, surface polished or turned; discs and ring blanks are supplied in forged state; ring parts are supplied in solution state; plates are supplied after solution, alkaline acid washing, straightening, and edge cutting; strips are delivered after cold rolling, solution, and descaling; wires are delivered in solution acid-washed coil or straight bar form, solution straight bar finely polished.
7. GH600 melting and casting process: The alloy is melted using one of the following processes: (1) non-vacuum induction melting plus electroslag remelting; (2) electric arc furnace melting plus electroslag remelting; (3) vacuum melting.
8. Overview of GH600 applications and special requirements: This alloy has mature usage experience abroad and has been made into aerospace engine components domestically, which have been tested through flight tests and are also starting to be used in aviation.
2.Physical and chemical properties of GH600:
1. Thermal properties of GH600:
(1) Melting temperature range of GH600: 1370~1430℃[1].
(2) Thermal conductivity of GH600: see Table 2-1.
Table 2-1[2]
| θ/℃ | 20 | 100 | 200 | 300 | 400 | 500 | 600 | 700 | 800 | 900 |
| λ/(W/(m·℃)) | 12.85 | 13.94 | 15.15 | 16.62 | 18.71 | 20.72 | 22.40 | 24.49 | 27.00 | 29.51 |
(3) Specific heat capacity of GH600: see Figure 2-1.
(4) Linear expansion coefficient of GH600: see Table 2-2.
2. Density of GH600: ρ=8.43g/cm3.
3. Electrical properties of GH600: resistivity see Figure 2-2.
Table 2-2[2]
| θ/℃ | 20-200 | 20-300 | 20-400 | 20-500 | 20-600 | 20-700 | 20-800 | 20-1000 |
| α/10-6℃-1 | 12.35 | 12.75 | 13.10 | 13.55 | 14.50 | 15.15 | 15.70 | 16.20 |
4. Magnetic properties of GH600: The alloy is non-magnetic.
5. Chemical properties of GH600: The oxidation rate of GH600 in air medium after 100 hours of testing is shown in Table 2-3.
Table 2-3[3]
| θ/℃ | 800 | 900 | 1000 |
| Oxidation rate/(g/m2·h) | 0.01865 | 0.05724 | 0.13718 |
Three,GH600 mechanical properties: The performance specified in the GH600 technical standard is shown in Table 3-1.
Table 3-1
| Variety | θ/℃ | Tensile properties | HBS | Bending test | |||
| σb/MPa | σP0.2/MPa | δ5/% | φ/% | ||||
| Bar | 20 | >=585 | >=240 | >=30 | - | 134~217 | - |
| Discs, ring blanks or ring-shaped parts | 20 | >=520 | >=205 | >=35 | - | >=187 | - |
| Hot-rolled plate | 20 | >=550 | >=240 | >=35 | >=40 | - | - |
| 900 | >=95 | >=45 | >=40 | >=50 | - | - | |
| Cold-rolled plate | 20 | >=550 | >=240 | >=30 | - | - | ① |
| 900 | >=90 | >=40 | >=60 | - | - | - | |
| Cold-rolled plate | 20 | >=550 | >=200 | >=30 | - | - | Testing |
| Strip | 20 | >=550 | >=240 | >=30 | - | - | ① |
| Wire | 20 | Actual measurement | Actual measurement | Actual measurement | - | HV≤151 | Cold top forging qualified |
① The supplied state of the plate should undergo a room temperature bending test, with the core rod diameter equal to the product thickness multiplied by the bending coefficient in Table 3-2. The bending axis should be parallel to the rolling direction. After bending 180°, it should be inspected under 20x magnification, and no cracks should be present.
Table 3-2
| Product thickness/mm | <0.25 | 0.25~1.30 | >1.30~4.00 |
| Bending coefficient | Mutual agreement | 1 | 2 |
Four,GH600 microstructure:
1. GH600 phase transformation temperature:
2. GH600 time-temperature-structure transformation curve:
3. GH600 alloy microstructure: After treatment at 1120℃ for 2 hours, only TiN nitrides and Cr7C3type carbides are present. After long-term aging at 870℃ for 1500 hours, the structure still contains Cr7C3and TiN, indicating that the alloy's structure is stable.
Five,GH600 process performance and requirements:
1. GH600 forming performance: The alloy has good hot working performance, with the forging heating temperature of the steel ingot being 1110~1140℃; the final forging temperature should not be less than 950℃, the heating temperature for slab rolling is 1130~1170℃, and the precision rolling heating temperature is 1090~1130℃. The solution treatment temperature for finished products is 1010~1050℃.
2. GH600 welding performance: The alloy has good welding performance and can be connected using various methods such as arc welding, argon arc welding, resistance welding, and brazing. Large or complex welded structures should be annealed at 870℃ for 1 hour after fusion welding to eliminate welding stress.
3. GH600 parts heat treatment process: The heat treatment process of the parts should be carried out according to the heat treatment system of the corresponding material standard. The annealing treatment of thin plates and strip parts should be conducted in a protective atmosphere.
Six,Specifications and supply status of GH600:
1. Variety classification: GH600 seamless pipes, GH600 welded pipes, GH600 plates, GH600 bars, GH600 forgings, GH600 rings, GH600 wires, and GH600 matching welding materials.
2. Delivery status: Seamless pipes: solution + acid pickling, length can be specified; plates: solution, acid washing, edge cutting; welded pipes: solution acid pickling + RT% flaw detection, forgings: annealed + turned; bars in forged state, surface polished or turned; strips delivered after cold rolling, solution soft state, and descaling; wires delivered in solution acid washed coil or straight bar form, solution straight bar fine polished state.
Previous Page
Previous Page
GH3044/GH44 nickel-based high-temperature alloy
Related Products
Product Consulting
Leave your contact information to get a free product quote!